si3525y0000a

Service information: Dome welding crack repair procedure for RT 390 axles

유형 si · 주제 35.25 · 버전 0100 · 2020-04-09

적용 대상: Model 400.243/281 with rear axle 400.780

“ko”(으)로는 제공되지 않아 영어(으)로 표시합니다.

위치

기능 그룹 2 섀시 › 35 뒷차축 › 35.25 액슬케이스 — 시리즈 400 (모델 243, 281, 780)

EinPAS 17 드라이브 트레인/액슬 › 17.51 뒤차축 › 17.51.50 하우징/액슬 튜브/캐리지/캐리어/토크 튜브 — 시리즈 400 (모델 243, 281, 780)

EinPAS 45 데이터/정보 › 45.20 정보/조치 › 45.20.20 서비스 정보 — 시리즈 400 (모델 243, 281, 780)

SI35.25-Y-0000A

Service information: Dome welding crack repair procedure for RT 390 axles

09.04.2020

Model

400.243/281 with rear axle 400.780

Service information: Dome welding crack repair procedure for RT 390 axles

Y35.25-A005-01

Service information: Dome welding crack repair procedure for RT 390 axles

Y35.25-A006-01

Service information: Dome welding crack repair procedure for RT 390 axles

Y35.25-A007-01

Service information: Dome welding crack repair procedure for RT 390 axles

A

Housing

B

Cover

C

First Weld Pass(Centered over fit-up line)

Y35.25-A008-06

Service information: Dome welding crack repair procedure for RT 390 axles

A

Housing

B

Cover

D

Second Weld Pass

Y35.25-A009-06

Service information: Dome welding crack repair procedure for RT 390 axles

A

Housing

B

Cover

E

Third Weld Pass

Y35.25-A011-06

Service information: Dome welding crack repair procedure for RT 390 axles

Y35.25-A010-01

A. Segment Classification:

HDT

B. Application:

Construction and Tractor Trailer

C. Specific Model:

2523C, 2528C, 3128C and 4928TT

D. Reason for change:

Dome welding crack repair procedure

E. Document Updating:

Will be updated in ASCENT

F. Part No Change:

NA

G. Cut Off Details For Series Implementation:

NA

H. Technical query:

Raise PCR for any technical complaints received on improved parts

For any clarifications, please write to [email protected] mentioning the circular reference number.

Thanking You

Yours Sincerely,

Customer Services - Technical Service

Daimler India Commercial Vehicle Pvt.Ltd.

Procedure For Repair Welding Of Dome Weld Crack

1

Scope : To provide instruction to repair axle housing having dome weld crack

The below procedure should be followed only, if

Crack located within the weld metal

The crack is <460 mm

2

Remove rear axle housing from the vehicle

3

Clean the axle housing throughly to get rid of the oil


Precaution
Thorough cleaning is required prior to welding

4

Place the axle housing between two V-Block

5

Mark A and A' on both the sides of the crack

6

Mark another extended mark B and B', which has to be 1 inch from the tail ends of the crack A and A'

This mark denotes the maximum limit for the rework procedure

The mark B and B' should be within the limit of 460mm

7

Grinding is done extensively on the cracked weld between B and B' ensuring the weld crack is fully removed

8

AWS E7018 / E7016 specification and recommended welding parameters provided by manufacturer is followed for this repair procedure

9

The electrodes are to be kept dry and preheated

About 300° Celsius per hour or as specified by the manufacturer

10

Initailly Arc welding root run is done using electrode E7018/2 mm diameter ensuring thorough root fusion

11

Subsequently additional weld layers are build up (Two or more layers to get uniform profile matching to the old weld run) using 4mm diameter

Remove the slag thoroughly and clean the weld deposit using steel wire brush on grinding before each pass of welding to avoid slag entrapments

12

Weld deposits to be made level with the adjacent original welding

13

Grind the surface. Ensure the complete weld is free from defects like blow holes, porosites, cracks etc.

14

Clean the internal portion of dome weld thoroughly to eliminate the oil presence and grind the internal surface to be fit for welding

15

Initially arc welding root run is done using electrode E7018 / 2 mm diameter

16

Subsequently additional weld layers are build up (Two or more layers to get uniform profile matching to the old weld run) using 2.4mm diameter

17

Grinding is done thoroughly to overcome weld slay / flux

18

After welding process reinstall rear axle housing to the vehicle


Precaution
Improper welding procedure deviating from the above may affect the safe performance of axle housing
Welding ground cable to be connected in such a way that it should not give any harmful effect to basic housing body