ra03323640050x

0050 - Recognizing dust damage to pistons and cylinder walls or liners Engines OM 364, 366 A/LA

Type ra · emne 03.00 · version 9581 · 1995-08-04

Gælder for:

Ikke tilgængelig på “da”; vises på Engelsk.

Placering

Funktionsgruppe 1 Motor › 03 Drivværk › 03.00 Generelt — Serie 364 (modeller 900, 901, 907, 954)

Gælder også for motorer/gearkasser: 356 940, 356 984, 366 900, 366 901, 366 905, 366 906, 366 907, 366 909, 366 910, 366 913, 366 914, 366 918, 366 919, 366 930, 366 931, 366 932, 366 933, 366 935, 366 936, 366 937, 366 938, 366 940, 366 944, 366 945, 366 946, 366 951, 366 952, 366 953, 366 960, 366 962, 366 966, 366 967, 366 968, 366 969, 366 970, 366 971, 366 973, 366 974, 366 975, 366 976, 366 978, 366 979, 366 980, 366 983, 366 988, 366 990, 366 992, 366 993, 366 994, 366 995, 366 997

03-0050 Recognizing dust damage to pistons and cylinder walls or liners

Note

If excessive oil consumption exists or in the event of engine failure, it is often unclear whether dust damage or normal wear and tear exists.

Possibility of recognizing problem

Severe dust deposits in the elbows of the intake passages at the clean air end (between air cleaner and engine) are a reliable indication of dust damage. A very fine film is permissible on engines with an oil bath air filter.

The shank wear pattern of a piston and the honing pattern of the cylinder also provide indications of damage caused by excessive dust levels.

0050 - Recognizing dust damage to pistons and cylinder walls or liners          
	Engines OM 364, 366 A/LA

Piston without dust damage

The shank wear pattern of the piston is characterized by its large area and the machining grooves are still clearly visible within this area.

Note

The machining grooves around the circumference are intentional recesses which are filled with oil and contribute to improved lubrication.

0050 - Recognizing dust damage to pistons and cylinder walls or liners          
	Engines OM 364, 366 A/LA

Piston with dust damage

The wear pattern on the shank has a mat appearance (as if rubbed with pumice stone) and the machining grooves are completely worn away within the contact area. In this advance stage, there are already slight fretting streaks on the shank and the piston rings are sharp-edged.

0050 - Recognizing dust damage to pistons and cylinder walls or liners          
	Engines OM 364, 366 A/LA

Cylinder walls and liners without dust damage

The honing is visible over the entire contact surface - more or less clearly depending on the type of engine. The honing may be partially worn away at the reversal point of the first piston ring.

0050 - Recognizing dust damage to pistons and cylinder walls or liners          
	Engines OM 364, 366 A/LA

Cylinder walls and liners with dust damage

The signs of machining from honing are either no longer visible at all or only very weakly.

In this advanced stage, a wear shoulder can be felt at the reversal point of the first piston ring. Poor sealing of the intake passages at the clean and unfiltered air ends (upstream and downstream of the air cleaner ), grooves or chafing points at the intake hose, sharply increased dust deposits, entraining of dirty oil from the oil bath air filter (if excessive quantity of oil), installation of non-approved start pilot systems and such like may cause dust damage.

When performing maintenance work, therefore, carefully inspect all the intake passages and connections so that concealed leak points or cracks are also detected.